Heat treatment is controlled heating and cooling of a metal to alter its physical (and sometimes chemical) properties; for steel, each process (annealing, normalising, stress relieving, hardening by quenching, tempering, austempering and martempering, case hardening) is defined by where it heats relative to the lower (A₁) and upper (A₃) critical temperatures on the Fe-Fe₃C diagram and how fast it cools.
An outline written by upsc.help, not an official UPSC answer; every fact checked by a separate review. How we work
What the question asks
The question has three parts: a definition, the purposes, and an explanation of processes tied to the iron-carbon diagram. A good answer sketches the steel portion of the Fe-Fe₃C diagram (eutectoid at 727 °C and 0·76% C), names the phases (ferrite, austenite, cementite, pearlite) and then places each process on it, adding martensite and bainite, which come from non-equilibrium cooling.
Answer outline
Introduction
Heat treatment: heating a metal or alloy and cooling it in a controlled way to alter its physical, and sometimes chemical, properties. Steel responds strongly because iron is allotropic: body-centred cubic ferrite changes to face-centred cubic austenite on heating (in pure iron, austenite exists from about 912 °C to 1394 °C).
Purposes
- Relieve internal stresses.
- Soften for cold working and improve machinability; make grain size uniform.
- Increase hardness and strength (hardening by quenching); restore toughness (tempering).
- Give a hard surface over a tougher core (case hardening).
- Improve electrical conductivity or magnetic properties.
Phases on the Fe-Fe₃C diagram
- Ferrite (α): BCC, holds at most about 0·02% C, soft and ductile.
- Austenite (γ): FCC, dissolves up to 2·03% C at 1146 °C; in plain-carbon steel it exists above the eutectoid temperature of 727 °C.
- Cementite (Fe₃C): about 6·67% C, hard and brittle.
- Pearlite: lamellar ferrite plus cementite formed from austenite of eutectoid composition (0·76% C) as it cools below 727 °C.
- Critical temperatures: lower A₁ (eutectoid line) and upper A₃.
Processes placed on the diagram
- Full annealing: heat above the upper critical temperature, then cool very slowly; this softens the steel.
- Normalising: heat above the upper critical temperature, cool in open air; more uniform grain size than annealing.
- Spheroidising: very slow cooling or long holding gives spherical cementite particles in ferrite (spheroidite).
- Stress relieving: heat below the lower critical temperature and cool uniformly.
- Hardening: austenitise and quench; austenite transforms by a diffusionless change to martensite (body-centred tetragonal, supersaturated with carbon), very hard and brittle.
- Tempering: reheat the quenched steel below the lower critical temperature (commonly about 205 to 595 °C); carbide size and distribution change, toughness rises, hardness falls.
- Austempering and martempering: quench into a bath and hold; austempering gives bainite, martempering gives martensite with less distortion, usually tempered afterwards.
- Case hardening: carbon or nitrogen is diffused into the surface; induction and flame hardening heat only the surface before quenching.
Diagram to draw
- Steel region of Fe-Fe₃C with the A₁ and A₃ lines and the eutectoid point (727 °C, 0·76% C); mark bands for annealing and normalising (above the upper critical line) and for stress relieving and tempering (below A₁).
- Note that martensite is not shown on the equilibrium diagram; martensite and bainite are read from TTT or CCT diagrams.
Conclusion
Heat treatment uses the phase changes shown on the iron-carbon diagram, with cooling rate as the second control: slow cooling gives equilibrium ferrite-pearlite structures, fast quenching gives martensite, which tempering then makes tougher.
Examples and data to cite
- Steels needing more strength than toughness, such as tools, are usually not tempered above about 205 °C.
- Springs are tempered so that they can deform elastically without breaking.
Facts to remember
- Eutectoid point of Fe-Fe₃C: 727 °C, 0·76% C.
- Maximum carbon in austenite: 2·03% at 1146 °C; in ferrite: about 0·02%.
- Cementite Fe₃C contains about 6·67% C.
- Martensite is a body-centred tetragonal phase supersaturated with carbon, formed by diffusionless transformation on quenching austenite.