A glass-epoxy composite consists of full length fibers of E-glass with modulus 72·5 GPa embedded in epoxy matrix with modulus 3·5 GPa. The volume percentage of glass fibers is 35%.
Compute :
(i) The modulus of elasticity of the composite in longitudinal and transverse directions.
(ii) The strain sustained by fibers and matrix, if a stress of 50 MPa is imposed on a cross-sectional area of 250 mm².
10 marks · directive: Compute
The core of a good answer
Rule of mixtures gives E_L = 0·35(72·5) + 0·65(3·5) = 27·65 GPa and inverse rule E_T = 5·25 GPa; under 50 MPa along the fibres both phases share the strain 50/27650 = 1·81 × 10⁻³ (fibre stress 131 MPa, matrix 6·3 MPa).
An outline written by upsc.help, not an official UPSC answer; every fact checked by a separate review. How we work
What the question asks
Continuous aligned fibre composite: isostrain (Voigt) loading along the fibres and isostress (Reuss) loading across them. For part (ii) the usual reading is longitudinal loading, where fibre and matrix strains are equal; the transverse case is added for completeness.
Answer outline
Introduction
E_f = 72·5 GPa, E_m = 3·5 GPa, V_f = 0·35, V_m = 0·65. Load = 50 MPa × 250 mm² = 12·5 kN.
Step 1: Longitudinal modulus
- E_L = V_fE_f + V_mE_m = 25·375 + 2·275 = 27·65 GPa
Step 2: Transverse modulus
- 1/E_T = V_f/E_f + V_m/E_m = 0·004828 + 0·185714
- E_T = 5·25 GPa
Step 3: Strain under longitudinal stress
- ε = σ/E_L = 50/27650 = 1·808 × 10⁻³, equal in fibre and matrix
- σ_f = 72500 × 0·001808 = 131·1 MPa; σ_m = 3500 × 0·001808 = 6·33 MPa
- Loads: fibres 11·47 kN, matrix 1·03 kN (fibres carry 92% of 12·5 kN)
Step 4: If the stress were transverse
- Isostress: ε_f = 50/72500 = 6·9 × 10⁻⁴, ε_m = 50/3500 = 1·43 × 10⁻²; composite strain 9·53 × 10⁻³
Conclusion
E_L = 27·65 GPa, E_T = 5·25 GPa; for 50 MPa along the fibres the strain in both fibre and matrix is 1·81 × 10⁻³. Check: σ_fV_f + σ_mV_m = 45·9 + 4·1 = 50 MPa. (Recomputed in Python.)
Examples and data to cite
- Glass fibre reinforced plastic with E-glass fibres in epoxy or polyester is used for boats and for GRP and GRE pipes.
- Because E_L is much larger than E_T, layers are laid with fibres in several directions to control the overall stiffness.
Facts to remember
- Equal-strain (Voigt) rule of mixtures: E_c = V_fE_f + V_mE_m, upper bound, models axial loading.
- Equal-stress (Reuss) inverse rule: 1/E_c = V_f/E_f + V_m/E_m, lower bound, models transverse loading.
- Under longitudinal load, F_f/F_m = E_fV_f/(E_mV_m).
- Strain = stress/modulus for linear elastic phases.